Abstract:
Radioisotope thermoelectric generator (RTG) plays an irreplaceable role in deep space exploration. The thermoelectric properties of silicon-germanium alloys have an important effect on the performance of RTG. The thermoelectric properties of silicon-germanium alloys are closely related to their preparation processes, impurity doping, so the preparation processes need to be optimized. P type Si
80Ge
20B
1.2 alloy were prepared by melting and hot pressing sintering,the effects of hot-pressing sintering process parameters on the density of Si
80Ge
20B
1.2 alloy were studied, the phase structure and microstructure, as well as the thermoelectric properties of Si
80Ge
20B
1.2 alloy were investigated. The results show that silicon and germanium can form a solid solution after smelting at 1 703 K for 2 h, the hot-pressing temperature has a more significant effect on the density of Si
80Ge
20B
1.2 alloy. The Si
80Ge
20B
1.2 was sintered at 1 523 K for 120 min under a pressure of 60 MPa has a density of 2.99 g/cm
3, reaching 99.7% of its theoretical density, XRD and SEM analysis showd that its structure is dense, silicon and germanium is evenly distributed; it has a good thermoelectric performance, thermal conductivity of 2 W/(m·K)-3,2W/(m·K) at the range of 303 K-1 073 K, power factor of 1.76 mW/(m·K
2) and
ZT value of 0.86 at 1 073 K. The results provide a reference for the development of thermoelectric generators in RTG.